This investigation evaluates colloidal silica pretreatment of recycled concrete aggregate (RCA) used as a 100 percent replacement for virgin coarse aggregate. RCA was presoaked with water or alumina-modified colloidal silica dispersions having average particle diameters of 11 and 34 nm. Fresh properties, compressive strength, and bulk electrical resistivity were compared with virgin-aggregate and untreated-RCA controls. Water presoaking restored slump to the virgin-aggregate reference, while selected colloidal silica treatments improved hardened properties. The highest-performing mixture achieved 51.4 MPa at 28 days, approximately 26 percent above untreated RCA, and increased electrical resistivity by more than 55 percent. These findings support further evaluation of RCA as a carrier for hydration-enhancing silica, while long-term durability and field performance remain to be verified.